Generic Name: 聚偏二氟乙烯 (PVDF) - 提供方: Arkema High Performance Polymers
Kynar Flex? resins are fluorinated thermoplastic copolymers.
Kynar Flex? 3120-50 is a pelletized flexible, semi-crystalline VF2 based copolymer. It can be molded or extruded and has a useful temperature range from -40°C - 150°C. Kynar Flex? 3120-50 has a UL RTI of 150°C.
Kynar Flex? 3120-50 can be used in compounding for cross-linkable wire and cable as well as both wire applications requiring low temperature flexibility and high temperature resistance.
Kynar Flex? 3120-50 also finds use as a polymer processing aid (PPA) for polyolefins. The use of Kynar Flex? 3120-50 or Kynar Flex 3121-50 at 200 -1000 ppm levels reduces extruder pressure, improves surface finish, reduces die build up, and improves gauge control.
與典型值比較 - Upgrade to compare! 與黃卡比較
單位: SI
總覽
材料狀態(tài)
已商用:當(dāng)前有效
資料 1Technical Datasheet (English)
UL 黃卡 2E54699-534488
搜索 UL 黃卡Arkema High Performance Polymers
供貨地區(qū)北美洲
非洲和中東
拉丁美洲
歐洲
亞太地區(qū)
添加劑熱穩(wěn)定劑
紫外線穩(wěn)定劑
特性半結(jié)晶
低溫下的柔性
共聚物
光穩(wěn)定
可交聯(lián)
良好的柔韌性
耐熱性,高
熱穩(wěn)定性
用途電線電纜應(yīng)用
混料
塑料改性
形式粒子
加工方法復(fù)合
擠出
型材擠出成型
注射成型
物理性能額定值
單位制
測試方法
密度 / 比重1.75 到 1.77
g/cm3
ASTM D792--1.78
g/cm3
ISO 1183熔流率(熔體流動(dòng)速率) (230°C/12.5 kg)2.5 到 7.5
g/10 min
ASTM D1238熔融體積流量(MVR) (230°C/10.0 kg)0.50
cm3/10min
ISO 1133吸水率0.030 到 0.050
%
ASTM D570飽和, 23°C0.030
%
ISO 62機(jī)械性能額定值
單位制
測試方法
拉伸模量689 到 1170
MPa
ASTM D638--700
MPa
ISO 527-1抗張強(qiáng)度24.1 到 34.5
MPa
ASTM D638屈服27.0
MPa
ISO 527-2斷裂, 23°C34.5 到 48.3
MPa
ASTM D638伸長率10 到 20
%
ASTM D638屈服15
%
ISO 527-2斷裂, 23°C300 到 500
%
ASTM D638標(biāo)稱拉伸斷裂應(yīng)變> 50
%
ISO 527-2彎曲模量 (23°C)621 到 827
MPa
ASTM D790彎曲強(qiáng)度 (5.0% 應(yīng)變, 23°C)20.7 到 34.5
MPa
ASTM D790壓縮強(qiáng)度 (23°C)31.0 到 41.4
MPa
ASTM D695摩擦系數(shù) 40.30
0.31
16.0 到 19.0
mg
內(nèi)部方法沖擊性能額定值
單位制
測試方法
簡支梁缺口沖擊強(qiáng)度 (23°C)無斷裂
無斷裂
無斷裂
額定值
單位制
測試方法
肖氏硬度 (邵氏 D, 23°C)65 到 70
額定值
單位制
測試方法
載荷下熱變形溫度54.4 到 76.7
°C
ASTM D6481.8 MPa, 未退火 543.3 到 54.4
°C
ASTM D6481.8 MPa, 未退火50.0
°C
ISO 75-2/A玻璃轉(zhuǎn)化溫度-41.1 到 -39.4
°C
ASTM D7028-- 6-40.0
°C
ISO 11357-2熔融溫度165
°C
ISO 11357-3--161 到 168
°C
ASTM D3418線形熱膨脹系數(shù) - 流動(dòng) (23°C)1.3E-4 到 1.9E-4
cm/cm/°C
ASTM D696比熱745 到 958
J/kg/°C
DSC導(dǎo)熱系數(shù)0.14 到 0.18
W/m/K
ASTM D433RTI Elec150
°C
UL 746BRTI Imp150
°C
UL 746BRTI150
°C
UL 746B電氣性能額定值
單位制
測試方法
表面電阻率 (23°C)5.3E+11 到 5.5E+11
ohms
ASTM D257介電強(qiáng)度 (23°C)51 到 59
kV/mm
ASTM D149介電常數(shù) (1 kHz)3.20 到 10.2
0.020 到 0.19
額定值
單位制
測試方法
可燃性等級(jí)V-0
5VA
V-0
42
%
ASTM D2863--43
%
ISO 4589-2光學(xué)性能額定值
單位制
測試方法
折射率 71.410
額定值
單位制
測試方法
熔體粘度 (230°C, 100 sec^-1)2000 到 2600
Pa·s
ASTM D3835補(bǔ)充信息額定值
單位制
測試方法
熱分解溫度375
°C
410
°C